Heap leaching is a low-cost method of treating low-grade ore. Crushed ore is stacked on a lined pad, typically many metres high, and a dilute cyanide solution (for gold) or acid (for copper) is applied to the surface by sprinklers or drippers. The solution percolates through the ore over weeks or months, dissolving the metal, and drains from the base for collection. A column test reproduces this at laboratory scale: ore crushed to the planned size is loaded into a column a few metres tall, solution is applied at the planned rate, and the solution leaving the base is measured daily.
Column tests are the principal design tool for heap leach projects, and crush size, agglomeration, reagent strength, application rate and leach cycle are all set from them. This article covers the procedure, the calculations and the step most often done incorrectly: scaling the leach time from a 2 m column to a heap many metres high.
Test procedure
- Prepare the ore at the planned crush size and measure the head grade on several splits.
- Agglomerate if fines would impede percolation: mix the ore with cement and lime (or acid, for copper) and water, cure for the planned time, and confirm that the agglomerates remain intact when wet.
- Load the column gently to avoid compaction, record the ore mass and height, and calculate the bulk density.
- Irrigate with barren solution at the design application rate, using a metering pump.
- Collect and measure the pregnant solution daily: volume, pH, free cyanide (or acid) and gold or metal concentration.
- At the end of the test, rinse and drain the column, then unload, dry, weigh and assay the residue, by size fraction where possible, and record the final moisture and any slumping of the ore column.
Application rate and solution-to-ore ratio
where
- application rate: solution per hour per square metre of surface (L/h·m²)
- ,
- solution flow (L/h) and irrigated area (m²)
- solution to ore ratio: total solution applied per tonne of ore (m³/t, the same as L/kg)
- dry ore mass (t)
- time a heap needs to receive the same ratio (h; divide by 24 for days), with the rate in m³/h·m²
- ,
- lift height (m) and bulk density of the stacked ore (t/m³)
Worked example: a 200 mm diameter column (area 0.0314 m²) holds 2.0 m of ore at a bulk density of 1.6 t/m³, or about 100.5 kg. At 10 L/h per m², the pump delivers 0.314 L/h, or 7.54 L/d. After 60 days the ore has received 7.54 × 60 = 452 L, a ratio of 452 ÷ 100.5 = 4.5 m³/t.
Calculating extraction
where
- ,
- volume (L) and gold concentration (mg/L) of each day's pregnant solution, including the final rinse
- ,
- residue gold grade (g/t, the same as mg/kg) and dry ore mass (kg)
| Day | 5 | 10 | 20 | 30 | 45 | 60 |
|---|---|---|---|---|---|---|
| Solution to ore ratio (m³/t) | 0.37 | 0.75 | 1.50 | 2.25 | 3.37 | 4.50 |
| Cumulative gold extraction (%) | 38 | 55 | 68 | 74 | 78 | 80 |
The column held 100.5 kg of ore at 0.80 g/t, or 80 mg of gold, and the residue assays 0.16 g/t (16 mg). Final extraction is (80 − 16) ÷ 80 = 80%, and the gold collected in solution should total about 64 mg. If it does not, the solution assays, residue assays and head grade should all be checked before either figure is relied on.
Scale-up from column to heap
A heap lift is considerably taller than a column. Each square metre of an 8 m lift carries 8 × 1.6 = 12.8 t of ore, compared with 3.2 t under each square metre of the 2 m column, so at the same application rate the heap receives solution per tonne four times more slowly.
To reach the column's 4.5 m³/t at 10 L/h per m² (0.24 m³/d per m²), the time required is t = 4.5 × 12.8 ÷ 0.24 = 240 days rather than 60. The heap needs four times the leach time to reach the same extraction, because extraction follows the solution applied per tonne. For this reason extraction curves are plotted against the solution-to-ore ratio, and leach cycles and solution inventories are set from that ratio.
Further scale-up allowances are set from experience with similar ores and site conditions. Heaps usually achieve somewhat lower extraction than columns, because of channelling, uneven irrigation and compaction under load. Field reagent consumption often differs from column results, through evaporation, dilution by rainfall and longer contact with reactive minerals. Tall columns, or columns loaded under pressure to simulate heap height, test whether percolation is maintained under the weight of the heap.
Recommended practice
Duplicate columns should be run, together with columns at two or three crush sizes, because crush size is usually the largest cost lever. A bottle roll on the same ore crushed finer provides a reference for the maximum achievable extraction (see our article on the bottle roll test).
Ponding on the top of the column and slumping of the ore both indicate permeability problems that will be more severe in the heap. Reagent consumption should be tracked per tonne and per day, as it often has a greater effect on operating cost than extraction does.
Glossary
- Heap leaching
- Leaching crushed ore stacked on a lined pad by trickling solution through it.
- Column test
- A laboratory or pilot test that leaches ore in a tall column to imitate a heap.
- Application rate
- Solution applied per hour per square metre of heap surface (L/h·m²).
- Solution-to-ore ratio
- Total solution applied per tonne of ore (m³/t).
- Agglomeration
- Binding fines to coarse particles with cement or acid and water so the heap stays permeable.
- Pregnant solution
- Solution draining from the heap carrying dissolved metal.
- Lift
- One layer of ore stacked on a heap.
- Channelling
- Solution flowing down preferred paths and bypassing parts of the ore.
Frequently asked questions
How is the solution-to-ore ratio calculated?
Sum all the solution applied and divide by the dry mass of ore. Expressed in L/kg or m³/t, the value is the same.
Why are column results plotted against the solution-to-ore ratio?
Extraction depends on how much solution each tonne of ore has received. A heap taller than the column receives solution per tonne more slowly, so it needs more days to reach the same extraction.
How long should a column test run?
Until extraction levels off, often 60 to 120 days or more, depending on the ore and crush size.
Do heaps achieve column extraction?
Usually somewhat less, because of channelling, compaction and uneven irrigation. Designers apply a deduction based on experience with similar ores.
Discuss your plant with a metallurgist
Tiegel is a Perth metallurgy company. We help with testwork, plant optimisation, metal accounting and investigations, and we build the Tiegel Suite software.
Talk to a metallurgistReferences and further reading
- Marsden, J.O. and House, C.I. (2006). The Chemistry of Gold Extraction, 2nd edition. Society for Mining, Metallurgy and Exploration.
- Kappes, D.W. (2002). Precious metal heap leach design and practice. In Mular, A.L., Halbe, D.N. and Barratt, D.J. (eds), Mineral Processing Plant Design, Practice, and Control. Society for Mining, Metallurgy and Exploration.
Worked examples and charts marked illustrative use invented figures, not data from any operation.