Bottle roll cyanide leach testing: procedure, extraction and reagent consumption

How a bottle roll cyanide test is run, and how to calculate gold extraction, the calculated head, and cyanide and lime consumption, with a worked example.

· 6 minute read · By

The bottle roll test is the standard laboratory leach test in gold metallurgy. One to two kilograms of ground ore is placed in a plastic bottle with water, lime and cyanide, and the bottle is rolled so that the slurry remains mixed and in contact with air. Solution samples taken over one to two days track the dissolution of gold, and at the end of the test the residue is assayed for the remaining gold. The test is used for scoping new deposits, for variability testing across an orebody, for optimising grind, cyanide strength and oxygen, and for investigating loss of recovery in an operating plant. This article sets out the procedure, the calculations in which small errors are common, and the interpretation of the results.

Test procedure

Bottle roll test stepsPrepare ore, make pulp and adjust pH with lime, add cyanide, roll, sample solution at set times, filter and assay the residue.Grind oreto plant P80Make pulplime to pH 10.5–11Add NaCNand rollSample at2, 4, 8, 24, 48 hFilter,assay residueeach sample: titrate free cyanide, measure pH and dissolved oxygen, assay gold in solutiontop up cyanide and lime back to target after each sample
The bottle roll test. Conditions are chosen to mimic the plant's leach, so the result predicts plant extraction and reagent use.
  1. Grind a representative split to the plant's target P80. Where the ore contains gravity gold, decide whether to remove it first so that the test reflects the plant flowsheet; our article on gravity recoverable gold testing discusses this.
  2. Add water, preferably site process water, to the planned pulp density, often 40 to 50% solids. In the worked example, 1,000 g of dry ore and 1,500 mL of water give 40% solids.
  3. Raise the pH to the target, typically 10.5 to 11, with lime before adding cyanide, so that cyanide is not lost as hydrogen cyanide gas. Record the lime added.
  4. Add cyanide to the target strength, for example 1.0 g/L sodium cyanide (NaCN), then start the timer and the rolls. Bottles are left open or vented, or oxygen is added, as specified in the test plan.
  5. At 2, 4, 8, 24 and 48 hours, stop the rolls, allow the solids to settle briefly and draw a small solution sample, 10 mL in the example. Filter the sample, assay it for gold and titrate it for free cyanide, and measure pH and dissolved oxygen in the bottle.
  6. After each sample, restore cyanide and lime to their targets and record every addition.
  7. At the end of the test, filter the whole pulp, wash the residue thoroughly, dry it and assay it for gold, normally in duplicate or triplicate. Assay the final solution.

Ores containing coarse gold require larger samples and multiple residue assays, because a single gold particle can change the result. Preg-robbing ores, which contain carbon that re-adsorbs dissolved gold, may require a carbon-in-leach version of the test with activated carbon added to the bottle.

Calculating gold extraction

Each solution sample removes some gold from the bottle, and the solution volume decreases slightly with each sample. Both must be accounted for:

Aj=cjVj+∑civi (earlier samples, i < j)calculated head=Afinal+r·MMXj=AjAfinal+r·M×100

where

Aj
gold dissolved by sample time j (mg)
cj, Vj
gold in solution at time j (mg/L) and solution volume in the bottle just before that sample (L)
ci, vi
gold concentration and volume (L) of each earlier solution sample taken out
r, M
residue assay (g/t, the same as mg/kg) and ore mass (kg)
Xj
gold extraction at time j (%)

Worked example, with no solution added back after sampling:

Time (h)Au in solution (mg/L)Volume before sample (L)Au in bottle (mg)Au removed in earlier samples (mg)Au dissolved (mg)Extraction (%)
20.621.5000.9300.0000.93049.4
40.851.4901.2670.0061.27367.6
81.021.4801.5100.0151.52480.9
241.181.4701.7350.0251.76093.4
481.211.4601.7670.0371.80395.8

The residue assays 0.08 g/t, which is 0.08 mg in 1 kg of ore. The calculated head is (1.803 + 0.08) ÷ 1.0 kg = 1.88 g/t, and extraction at 48 hours is 1.803 ÷ 1.883 = 95.8%. Ignoring the gold removed in samples would give 95.7% at 48 hours and would understate the early extractions slightly more, which is significant when leach rates are compared.

Gold extraction against leach timeExtraction reaches about 49% at 2 hours, 81% at 8 hours, 93% at 24 hours and 96% at 48 hours.020406080100081624324048Leach time (h)Gold extraction (%)Gold extraction: 0 → 0Gold extraction: 2 → 49Gold extraction: 4 → 68Gold extraction: 8 → 81Gold extraction: 24 → 93Gold extraction: 48 → 9695.8% at 48 h
Extraction curve from the worked bottle roll test, corrected for the gold removed in each solution sample. Illustrative figures.

The calculated head should be compared with the assayed head of the feed. Agreement within the expected assay precision supports the result. A calculated head well below the assay may indicate that gold was lost, for example by adsorption on the bottle or incomplete washing of the residue, or that the feed assay was biased by coarse gold.

Calculating cyanide and lime consumption

NaCN consumed=added−in solution−in samplesore mass

where

added, in solution, in samples
grams of sodium cyanide added, left in solution at the end, and removed in samples; dividing grams by kilograms of ore gives kg/t

In the example, 1.50 g NaCN was added at the start and 0.35 g and 0.20 g as top-ups, 2.05 g in total. At 48 hours the solution holds 0.62 g/L in 1.45 L, or 0.90 g, and the five samples removed about 0.04 g. Consumption = (2.05 − 0.90 − 0.04) ÷ 1.0 kg = 1.11 kg/t NaCN.

Lime consumption is calculated in the same way: lime added, less any measured residual alkalinity, divided by ore mass, and reported as kg/t of CaO or of the lime product used. The basis should be stated, because quicklime and hydrated lime differ in CaO content.

Laboratory consumption is a guide rather than a plant figure. Plants also lose cyanide in tailings solution, to cyanide destruction and through recycled water chemistry, and the ratio of plant to laboratory consumption is specific to each site.

Interpreting the results

Most free-milling ores release most of their gold within the first 8 to 24 hours. A curve still rising at 48 hours suggests coarse gold, slow-dissolving gold such as tellurides, or oxygen limitation.

Size-by-size residue assays and a diagnostic leach show whether undissolved gold is locked in sulphides, too coarse, or locked in silica.

High cyanide consumption indicates cyanide-consuming minerals, such as copper minerals, reactive sulphides including pyrrhotite, or oxidised ores with soluble salts.

Gold dissolution requires oxygen, and low dissolved oxygen slows the leach. Our article on oxygen in cyanide leaching covers this in more detail.

Common errors

  • Adding cyanide before raising the pH.
  • Failing to record small top-up additions, which are then omitted from the consumption figure.
  • Inadequate residue washing, which leaves dissolved gold in the filter cake and raises the residue assay.
  • A single residue assay on an ore containing coarse gold.
  • Comparing tests run at different pulp densities, cyanide strengths or grinds as though they were equivalent.

Glossary

Cyanidation
Dissolving gold in a dilute cyanide solution in the presence of oxygen.
Extraction
The fraction of gold in the ore that dissolved in the test.
Calculated head
The ore grade worked out from gold dissolved plus gold left in the residue.
Residue
The leached solids at the end of the test, filtered, washed and assayed.
Free cyanide
Cyanide not tied up in metal complexes, available to dissolve gold.
Protective alkalinity
The excess lime that keeps pH high enough to stop cyanide turning into hydrogen cyanide gas.
Preg-robbing
Re-adsorption of dissolved gold by natural carbon or clays in the ore.
Diagnostic leach
A sequence of leaches and acid digestions that shows where undissolved gold is locked.

Frequently asked questions

How long should a bottle roll test run?

Commonly 24 to 72 hours, with 48 hours a frequent choice. The test should run for at least the planned plant leach time, and longer if the extraction curve is still rising.

What pulp density is used in bottle roll tests?

Usually close to the plant's leach density, often 40 to 50% solids by mass. It should be kept constant across tests that are to be compared.

Why correct extraction for the solution samples?

Each sample removes dissolved gold from the bottle. Without the correction, gold dissolved early in the test is under-counted and extraction is understated, most noticeably at the early sample times.

Is laboratory cyanide consumption the same as plant consumption?

No. It shows the cyanide consumed by the ore itself under test conditions. Plant consumption also includes losses to tailings, detoxification and water recycling, and usually differs.

Discuss your plant with a metallurgist

Tiegel is a Perth metallurgy company. We help with testwork, plant optimisation, metal accounting and investigations, and we build the Tiegel Suite software.

Talk to a metallurgist

References and further reading

  1. Marsden, J.O. and House, C.I. (2006). The Chemistry of Gold Extraction, 2nd edition. Society for Mining, Metallurgy and Exploration.
  2. Fleming, C.A., Mezei, A., Bourricaudy, E., Canizares, M. and Ashbury, M. (2011). Factors influencing the rate of gold cyanide leaching and adsorption on activated carbon, and their impact on the design of CIL and CIP circuits. Minerals Engineering, 24(6), 484–494. Link
  3. Wills, B.A. and Finch, J.A. (2016). Wills' Mineral Processing Technology, 8th edition. Butterworth-Heinemann.

Worked examples and charts marked illustrative use invented figures, not data from any operation.