Carbon elution: AARL and Zadra stripping, bed volumes and elution efficiency

How gold is stripped from loaded carbon by AARL and Zadra elution, with calculations for bed volumes, eluate grade and elution efficiency.

· 4 minute read · By

In CIL and CIP plants, gold is recovered from solution onto activated carbon and must then be removed from the carbon. The loaded carbon is transferred to an elution column and treated with hot solutions that reverse the adsorption, transferring the gold into a small volume of eluate for electrowinning. The two common methods are AARL and Zadra, named after the laboratory and the researcher who developed them. Elution is a batch process governed by a small number of variables: the carbon mass, the bed volumes of solution, the temperature and the gold remaining on the carbon. This article describes both methods and the calculations for a strip, with a worked example.

AARL elution

AARL elution sequenceAcid wash, rinse, pre-soak in caustic cyanide, elution with hot water, cooling; eluate goes to electrowinning; carbon to regeneration.Acid washremove scaleRinsewaterPre-soakNaOH + NaCNElutehot waterCooland transferEluate toelectrowinningCarbon to kilnregeneration
The AARL (Anglo American Research Laboratories) elution sequence. Zadra elution instead recirculates hot caustic cyanide solution between the column and the electrowinning cells.
  1. Acid wash. Dilute hydrochloric acid removes calcium carbonate and other scale, which would otherwise block pores and reduce activity, and the carbon is then rinsed with water.
  2. Pre-soak. A caustic cyanide solution of sodium hydroxide and sodium cyanide is pumped into the column and left to soak at temperature, loosening the gold cyanide on the carbon.
  3. Elution. Hot, good-quality water, low in calcium and dissolved salts, is pumped through once at a temperature above 100 °C in a pressurised column. Gold transfers into the water, which becomes the eluate.
  4. Cooling and transfer. The column is cooled with water, the eluate is sent to electrowinning, and the carbon is sent to the kiln for regeneration.

AARL strips are relatively short, and the eluate is collected in a tank before electrowinning. Water quality is important, because calcium and magnesium in the elution water reduce stripping efficiency.

Zadra elution

In Zadra elution, a hot solution of sodium hydroxide and sodium cyanide circulates continuously from the column through the electrowinning cells and back, so gold is removed from solution as it is stripped. Atmospheric Zadra operates below boiling point and takes considerably longer, while pressure Zadra operates at higher temperature and is faster. The circuit is simpler to operate than AARL but has a longer cycle.

Elution calculations

BV=mcρcelution efficiency=Lloaded−LelutedLloadedgold stripped=mc×(Lloaded−Leluted)

where

BV
bed volume: the volume the carbon bed occupies (m³)
mc
mass of carbon in the column (t)
ρc
bulk density of the carbon bed (t/m³)
Lloaded, Leluted
gold on carbon before and after elution (g/t)

Worked example: a 6 t batch of loaded carbon assays 4,300 g/t gold. The carbon bed has a bulk density of about 0.5 t/m³, and after elution the carbon assays 60 g/t.

The bed volume is 6 ÷ 0.5 = 12 m³, so an elution of 8 bed volumes uses 96 m³ of eluant. Gold stripped = 6 × (4,300 − 60) = 25,440 g, or 25.4 kg. Elution efficiency = (4,300 − 60) ÷ 4,300 = 98.6%, and the average gold in eluate = 25,440 g ÷ 96 m³ = 265 g/m³ (265 mg/L).

Gold in eluate against bed volumesGold concentration peaks at about 720 mg/L in the second bed volume and falls below 50 mg/L by the seventh.0200400600800012345678Bed volumes of eluant passedGold in eluate (mg/L)Gold in eluate: 0 → 0Gold in eluate: 1 → 140Gold in eluate: 2 → 720Gold in eluate: 3 → 590Gold in eluate: 4 → 340Gold in eluate: 5 → 180Gold in eluate: 6 → 90Gold in eluate: 7 → 40Gold in eluate: 8 → 20Eluate gold
Elution profile for the worked example: 25.4 kg of gold in 8 bed volumes, an average of 265 mg/L. Most gold comes off in the first few bed volumes; the tail shows how complete the strip is. Illustrative figures.

The elution profile, gold in eluate plotted against bed volumes, shows the course of the strip. A sharp early peak and a low tail indicate a good strip. A low, flat profile indicates low temperature, an inadequate pre-soak, poor water quality or fouled carbon.

Eluted carbon grade

Carbon returned to the adsorption circuit with a high residual gold grade, for example 200 g/t rather than 50 g/t, begins each cycle partly loaded. It adsorbs less gold in the final tanks, so more gold leaves in the tailings solution, and the gold remaining on it forms part of gold in circuit. The eluted carbon grade should be recorded for every strip; see our articles on carbon testing and gold in circuit.

Routine strip checks

  • Loaded and eluted carbon assays for every strip, from well-mixed samples.
  • Column inlet and outlet temperatures, and the time at temperature.
  • Pre-soak cyanide and caustic strengths.
  • Elution water hardness, for AARL.
  • A gold balance, in which gold stripped from the carbon should agree with gold in eluate plus gold recovered in electrowinning, within sampling error.

Glossary

Elution
Stripping gold off loaded carbon into solution.
Eluate
The gold-rich solution produced by elution.
Eluant
The solution pumped through the carbon to strip it.
Bed volume
The volume occupied by the carbon bed; flows and volumes are expressed as multiples of it.
AARL
Anglo American Research Laboratories elution: acid wash, caustic cyanide pre-soak, hot water elution.
Zadra
Elution with hot caustic cyanide solution recirculating through the column and electrowinning cells.
Acid wash
Dilute hydrochloric acid treatment that removes scale from carbon.
Regeneration
Heating eluted carbon in a kiln to restore its activity.

Frequently asked questions

What is the difference between AARL and Zadra elution?

AARL uses an acid wash, a caustic cyanide pre-soak and a single pass of hot water, and the eluate is collected for electrowinning. Zadra recirculates hot caustic cyanide solution between the column and the electrowinning cells.

How is elution efficiency calculated?

Loaded carbon grade minus eluted carbon grade, divided by loaded carbon grade.

What is a bed volume in elution?

The volume occupied by the carbon bed, equal to the carbon mass divided by its bulk density. Flows and solution volumes are expressed as multiples of it.

What causes a high eluted carbon grade?

Common causes are low temperature, an inadequate pre-soak or elution time, weak pre-soak reagents, hard elution water in AARL, or carbon fouled with scale or organics.

Discuss your plant with a metallurgist

Tiegel is a Perth metallurgy company. We help with testwork, plant optimisation, metal accounting and investigations, and we build the Tiegel Suite software.

Talk to a metallurgist

References and further reading

  1. Marsden, J.O. and House, C.I. (2006). The Chemistry of Gold Extraction, 2nd edition. Society for Mining, Metallurgy and Exploration.
  2. Davidson, R.J. and Duncanson, D. (1977). The elution of gold from activated carbon using deionized water. Journal of the South African Institute of Mining and Metallurgy, 77.
  3. Zadra, J.B., Engel, A.L. and Heinen, H.J. (1952). Process for recovering gold and silver from activated carbon by leaching and electrolysis. US Bureau of Mines, Report of Investigations 4843.

Worked examples and charts marked illustrative use invented figures, not data from any operation.