The gold room produces the final product of a gold plant. Gold stripped from carbon and deposited in the electrowinning cells as sludge is dried, mixed with fluxes that dissolve impurities, and melted in a furnace. Gold and silver collect at the bottom of the crucible, the impurities form a glassy slag on top, and the metal is poured into moulds as doré bars for dispatch to a refinery. Because the gold room handles the most valuable material on site in its most portable form, it operates under strict security, with restricted access, camera coverage, two-person rules and weighing at every step.
This article covers the gold room process from electrowinning to bullion dispatch, the doré calculations and the gold room balance. The upstream steps are covered in carbon elution and electrowinning.
Sludge handling, drying and calcining
Gold deposited on steel wool or stainless steel mesh cathodes is washed off with high-pressure water and filtered. The wet cake can contain a third or more of its mass as water, which must be removed before smelting because water in a hot crucible boils violently. The cake is dried in an oven, and often calcined at a higher temperature to oxidise base metals and burn off organic material, which produces a cleaner smelt. Some plants smelt the cathodes directly.
Worked example: 80 kg of wet filter cake at 35% moisture gives 80 × (1 − 0.35) = 52 kg of dry sludge. A representative sample of the dry sludge assays 35% gold and 6% silver, so the furnace charge contains 18.2 kg of gold and 3.1 kg of silver.
Fluxing and smelting
The dry sludge is mixed with fluxes, typically borax, which dissolves metal oxides and lowers the melting point of the slag; silica, which forms a glassy slag; sodium nitrate, an oxidant that converts base metals to oxides; and in some cases sodium carbonate. The appropriate recipe depends on the composition of the sludge, particularly its copper, iron and zinc content, and is established by trial. The charge is melted in an induction or fuel-fired furnace well above the melting point of gold, 1,064 °C, so that both the metal and the slag are fully liquid and separate cleanly. The slag is skimmed or poured off first, and the bullion is then poured into bar moulds.
Doré calculations
where
- parts of gold per thousand parts of bullion by mass; doré is often several hundred, refined bars 995 or more
Worked example: the pour produces 22.6 kg of doré, and drill or pin samples from the bar assay 805 parts per thousand gold and 135 silver. Contained gold is 22.6 × 805 ÷ 1,000 = 18.19 kg, or 18,193 ÷ 31.1035 = 585 troy ounces. Contained silver is 3.05 kg, or 98 ounces.
The refinery assays the bar independently, and its result, subject to the agreed splitting limits and umpire procedures, determines the payment. Persistent differences between the mine's and the refinery's assays point to the sampling of the bars, which is difficult because gold and silver segregate as the bar cools.
The gold room balance
where
- gold in the dried sludge or cathode material fed to the furnace, from weight and assay
- the difference, which should be within the combined sampling and assay precision
| Item | Mass (kg) | Gold (kg) |
|---|---|---|
| Dry sludge in | 52.0 | 18.20 |
| Doré out, at 805 fineness | 22.6 | 18.19 |
| Slag out, at 0.12% gold | 9.0 | 0.011 |
| Accounted for | 18.20 (100.0%) |
A balance that closes within the combined precision of the sludge, bar and slag assays is the expected result. A persistent shortfall requires investigation, with unsampled spillage, gold retained in furnace linings and crucibles, dust losses and sampling bias on the sludge as the usual causes. In a gold room, an unexplained loss is also a security matter.
Slag and other gold-bearing residues
Slag always contains some gold, both as small droplets of metal (prills) and in solution in the slag. It is crushed, the prills are recovered by screening or gravity, and the remainder is usually returned through the mill or re-smelted. Crucibles, furnace linings, filter cloths and floor sweepings also contain gold and are stored and processed under the same controls.
Security and records
Access to the gold room is restricted to named personnel, and at least two people are present whenever gold is handled. Cameras cover every step, and the recordings are retained. Every weight, including sludge, fluxes, bars, slag and samples, is recorded and countersigned. Bars are numbered, stamped, weighed and sealed for dispatch and transported by a secure carrier, and the gold room balance for each pour is reviewed by someone outside the gold room team.
Glossary
- Doré
- An impure bar of gold and silver produced at the mine for refining.
- Fineness
- Gold content in parts per thousand by mass.
- Troy ounce
- The unit for precious metals: 31.1035 g.
- Flux
- Chemicals added to the furnace charge to dissolve impurities into a fluid slag.
- Calcining
- Heating in air to drive off water and oxidise base metals and organics before smelting.
- Slag
- The glassy layer of oxides and flux that separates from molten bullion.
- Prill
- A small droplet of metal trapped in slag.
- Gold room balance
- A reconciliation of gold into and out of the gold room for each pour.
Frequently asked questions
What is the difference between doré and refined gold?
Doré is the mine's product, a bar containing gold, silver and some base metals. A refinery separates the gold to 995 parts per thousand or higher.
How are grams converted to troy ounces?
Divide by 31.1035. For example, 18,193 g of gold is 585 troy ounces.
Why is slag recycled?
It always contains some gold, both as prills and in solution in the slag. Crushing it, recovering the prills and returning the remainder to the circuit recovers that gold.
Why must the sludge be dry before smelting?
Water in a hot crucible boils violently and can eject molten material. Drying or calcining also gives a more accurate weight and assay.
Discuss your plant with a metallurgist
Tiegel is a Perth metallurgy company. We help with testwork, plant optimisation, metal accounting and investigations, and we build the Tiegel Suite software.
Talk to a metallurgistReferences and further reading
- Marsden, J.O. and House, C.I. (2006). The Chemistry of Gold Extraction, 2nd edition. Society for Mining, Metallurgy and Exploration.
- LBMA. The Good Delivery Rules for Gold and Silver Bars.
Worked examples and charts marked illustrative use invented figures, not data from any operation.